LOCTITE ABLESTIK ABP 6892

Harmonization Code : 3506.10.00.00 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg

Fingerprint sensor bonding attach ABP 6892 LOCTITE ABLESTIK ABP 6892 LOCTITE ABLESTIK ABP 6892 LOCTITE ABLESTIK ABP 6892

Main features

  • Designed for Fingerprint Sensors
  • Low stress for ultra thin glass
  • Low outgassing and finest filler

Product Description

LOCTITE ABLESTIK ABP 6892 is a transparent, non-conductive BMI/acrylate die attach adhesive developed for low-stress sensor assembly and applications requiring robust mechanical properties. It is used for fingerprint and optical sensor assemblies, including ultra-thin glass or ceramic bonding on sensor dies up to 10 x 10 mm. Its low modulus, low viscosity, fine filler size below 10 um, and improved flow support thin bond-line processing below 15 um. ABP 6892 also provides high optical transmittance, a refractive index of 1.50 with reflow-resistant optical performance, and minimal resin bleed-out, making it suitable for evaluation where optical performance and tight bond-line control are important.

LOCTITE ABLESTIK ABP 6892 has also been used for protection of Au wire-bond balls around the edge of a semiconductor die. In this application, the material was applied by jetting, where its flow characteristics and low-temperature, relatively short cure profile supported the production process. Its combination of fine filler, controlled flow, and transparent cured appearance can also support evaluation for localized wire-bond protection and optical encapsulation applications.

Key features

  • Low-stress BMI/acrylate chemistry: Low-modulus cured behavior supports stress-sensitive sensor and thin-substrate assemblies.
  • Fine filler for thin bond lines: Filler size below 10 um and improved flow support bond-line thicknesses below 15 um.
  • Extended process window: 2-hour open time and 8-hour staging time, with a TDS work life of 24 hours at 25 C.
  • Low-temperature cure option: Recommended cure includes a 15-minute ramp to 80 C followed by a 60-minute hold.
  • High optical transmittance: Optical transmission remains high across the evaluated visible and near-infrared ranges, with performance dependent on wavelength, thickness, and thermal exposure.
  • Reflow-resistant optical properties: Refractive index of 1.50 with minimal resin bleed-out supports optical sensor and precision-bonding applications.
  • Environmental exposure performance: Robust adhesion and a void-free bond line were observed after 96 hours at 60 C/90% RH and 100 hours of HTS at 120 C under the evaluated conditions.

Applications / Suitable for

  • Fingerprint and optical sensor assemblies
  • Ultra-thin glass or ceramic sensor-die bonding
  • Sensor dies up to 10 x 10 mm
  • Thin bond-line applications below 15 um
  • Au wire-bond ball protection using jet dispensing
  • Optical encapsulation and localized sensor protection
Product Family

ABP6892/10C0

10CC EFD - 2089759
1. Select Package Type

Loading pricing…

Product availability
US Shipping in 30 days
CA Shipping in 12 weeks
EU Shipping in 12 weeks
Packaging
Unit of measure Syringe
Net weight 10.5 g
Gross weight 19.9 g
Dimensions 2.8 x 1.4 x 7 cm
TDS, SDS & Technical Documents

Technical Specifications

General Properties
Density (g)
1.05 g/cm3
Refractive index
The refractive index determines how much the path of light is bent, or refracted, when entering a material. It is calculated by taking into account the velocity of light in vacuum compared to the velocity of light in the material. The refractive index calculation can be affected by the wavelength of light and the temperature of the material. Even though it is usually reported on standard wavelengths it is advised to check the TDS for the precise test parameters.
1.503
Work life @25°C
Work life is the amount of time we have to work with a material until it is no longer able to be easily worked and applied on a substrate. It is based on the change in viscosity and it can rely on the application requirements.
24 hours
Thermal Properties
Glass Transition Temperature (Tg)
The glass transition temperature for organic adhesives is a temperature region where the polymers change from glassy and brittle to soft and rubbery. Increasing the temperature further continues the softening process as the viscosity drops too. Temperatures between the glass transition temperature and below the decomposition point of the adhesive are the best region for bonding. The glass-transition temperature Tg of a material characterizes the range of temperatures over which this glass transition occurs.
-24.6 °C
Physical Properties
Thixotropic index
Thixotropic Index is a ratio of a material s viscosity at two different speeds in Ambient temperature, generally different by a factor of ten. A thixotropic material s viscosity will decrease as agitation or pressure is increased. It indicates the capability of a material to hold its shape. Mayonnaise is a great example of this. It holds its shape very well, but when a shear stress is applied, the material easily spreads. It helps in choosing a material in accordance to the application, dispense method and viscosity of a material.
1.75
Viscosity
Viscosity is a measurement of a fluid’s resistance to flow. Viscosity is commonly measured in centiPoise (cP). One cP is defined as the viscosity of water and all other viscosities are derived from this base. MPa is another common unit with a 1:1 conversion to cP. A product like honey would have a much higher viscosity -around 10,000 cPs- compared to water. As a result, honey would flow much slower out of a tipped glass than water would. The viscosity of a material can be decreased with an increase in temperature in order to better suit an application
4,100 mPa.s

Additional Information

 
Non-Conductive Die Attach Adhesive

LOCTITE ABLESTIK ABP 6892

LOCTITE ABLESTIK ABP 6892 is a clear, non-conductive BMI/acrylate die attach paste developed for low-stress sensor assembly and applications requiring robust mechanical properties. The material is used for ultra-thin glass or ceramic bonding on sensor dies up to 10 x 10 mm and supports thin bond-line processing below 15 um. Its low modulus, low viscosity, fine filler size below 10 um, high optical transmittance, refractive index of 1.50 with reflow-resistant optical behavior, and minimal resin bleed-out support precision sensor and optical assembly applications.

ABP 6892 has also been used for localized protection of Au wire-bond balls around the perimeter of semiconductor die. Jet dispensing was used in this application, combining controlled material flow with a relatively low-temperature cure profile for production processing.

Clear paste BMI/acrylate chemistry Non-conductive Low modulus Fine filler below 10 um 80 C cure option High optical transmittance Halogen free
 
As-Supplied Material

Material and handling properties

The clear paste combines low-viscosity processing behavior with thixotropy and an extended work-life window. Fine filler below 10 um supports flow into thin bond-line and localized encapsulation geometries.

Typical as-supplied and storage data
Property Value Unit Method / condition
Technology BMI/Acrylate - As supplied
Appearance Clear paste - As supplied
Viscosity 4,100 mPa.s Brookfield, 25 C, 0.5 rpm
Thixotropic index 1.75 - Typical value
Work life 24 hours 25 C
Shelf life 365 days Stored at -40 C from date of manufacture
 
Processing

Workability, thin bond lines and cure

ABP 6892 combines extended material work life with application-specific open and staging windows. Its fine filler and flow behavior support thin bond lines below 15 um, while two recommended heat-cure profiles provide processing flexibility.

Application window

Open time: 2 hours. Staging time: 8 hours. TDS work life: 24 hours at 25 C. These process windows should be treated separately.

Thin bond-line processing

Fine filler below 10 um and improved flow support thin bond-line assemblies below 15 um for ultra-thin glass, ceramic and sensor constructions.

80 C cure profile

Ramp for 15 minutes to 80 C, then hold for 60 minutes.

130 C cure profile

Ramp for 15 minutes to 130 C, then hold for 30 minutes.

Cure guidance: The cure profiles are guideline recommendations. Cure time and temperature may require adjustment for the application, curing equipment, oven loading and actual material temperature.

 
Storage and Handling

Thawing and dispensing controls

  1. Allow the container to reach room temperature before use.
  2. After removal from frozen storage, keep syringes standing vertically while thawing.
  3. Do not open the container until the contents reach 25 C. Remove any moisture from the exterior before opening.
  4. Do not re-freeze the adhesive after it has thawed to 25 C.
  5. Place thawed adhesive on dispense equipment for use. When transferring material to another reservoir, minimize air and contaminant entrapment.
  6. Use the adhesive within the applicable work-life window.
 
Cured Material

Low-modulus mechanical and thermal behavior

The cured adhesive has a glass transition temperature below room temperature and strongly temperature-dependent modulus. Tensile modulus is 176 MPa at 25 C, decreasing to 28 MPa at 100 C and 24 MPa at 150 C.

Typical cured-material properties
Property Value Unit Method / condition
Glass transition temperature -24.6 C TMA
CTE below Tg 111.4 ppm/C Below Tg
CTE above Tg 190.6 ppm/C Above Tg
Moisture absorption 0.44 % 85 C / 85% RH
Outgassing during cure 0.7 % During cure
Thermal conductivity 0.22 W/mK Test method not specified in supplied application data
Refractive index 1.50 - Reflow-resistant optical behavior

Temperature-dependent tensile modulus

Test temperature Tensile modulus Unit Method
-65 C 1,912 N/mm2 DMTA
25 C 176 N/mm2 DMTA
100 C 28 N/mm2 DMTA
150 C 24 N/mm2 DMTA
250 C 34 N/mm2 DMTA

Die shear on glass

Test configuration Temperature Die shear
3 x 3 mm Si die on glass 25 C 13 kg-f/die
3 x 3 mm Si die on glass 80 C 6 kg-f/die

These values are typical characterization data rather than guaranteed product specifications. Mechanical performance depends on the tested materials, bond-line geometry, cure condition, test temperature and assembly construction.

 
Application Fit

Transparent low-stress bonding and localized protection

Ultra-thin glass or ceramic bonding

ABP 6892 is positioned for transparent low-stress bonding of ultra-thin glass or ceramic on sensor dies up to 10 x 10 mm. Improved flow and fine filler below 10 um support bond-line thicknesses below 15 um.

Optical sensor and encapsulation evaluation

High optical transmittance, a refractive index of 1.50 with reflow-resistant behavior, low modulus and minimal resin bleed-out support evaluation where the cured adhesive lies within or close to an optical path.

Au wire-bond protection by jetting

ABP 6892 has been used to protect Au wire-bond balls around the edge of semiconductor die. Jet dispensing provided localized material placement while the low-temperature cure profile supported the associated production process.

 
Optical Performance Evidence

Transmission across visible and infrared wavelengths

ABP 6892 has been characterized across both the visible/near-infrared region and an extended wavelength range to 2500 nm. The results show that optical performance depends on wavelength, adhesive thickness and thermal history, so application assessment should focus on the actual operating wavelength and expected bond-line thickness.

Visible transmission, thickness and thermal aging

LOCTITE ABLESTIK ABP 6892 visible transmission versus adhesive thickness and temperature aging

Transmission from 800 to 2500 nm

LOCTITE ABLESTIK ABP 6892 optical transmission spectrum from approximately 800 to 2500 nanometers

Visible-spectrum 

For specimens cured for 60 minutes at 80 C, transmission at 400 nm decreases from 95.73% at an actual thickness of 21 um to 94.89% at 55 um and 93.09% at 104 um. At 900 nm, the corresponding transmission values remain 100%, 99.88% and 99.84%. The thickness effect is therefore substantially more pronounced near 400 nm than at 900 nm.

Application implication: Bond-line thickness becomes particularly important when the optical system operates near the short-wavelength edge of the visible spectrum. A thinner and well-controlled adhesive layer can preserve more transmission around 400 nm, while applications operating closer to 900 nm are less sensitive to the thickness variation represented by this dataset.

Thermal-aging context: The thermal-aging curves use approximately 160 to 170 um thick specimens exposed for seven days at 85 C or 150 C. The higher-temperature exposure produces the larger shift of the short-wavelength transmission edge toward longer wavelengths. Because these specimens are substantially thicker than the 21 to 104 um thickness series, the aging curves should not be directly converted into quantitative predictions for a thin die-attach bond line.

Extended-spectrum 

 Transmission is generally high through portions of approximately 800 to 1600 nm, but it is not spectrally uniform. Distinct absorption regions appear around approximately 1200 nm, 1400 nm, 1700 to 1800 nm, 2100 nm and 2300 to 2450 nm.

Application implication: A transparent appearance or strong transmission at 850 to 940 nm does not establish equivalent transmission at every near-infrared or short-wave infrared wavelength. Optical sensor and emitter designs should therefore assess ABP 6892 at the specific wavelength used by the device, particularly when that wavelength is near one of the absorption regions.







Transmission by adhesive thickness

Transmission after 60-minute cure at 80 C
Nominal thickness Actual thickness Transmission at 400 nm Transmission at 900 nm
15 um 21 um 95.73% 100%
50 um 55 um 94.89% 99.88%
100 um 104 um 93.09% 99.84%

Optical-data qualification: Optical performance depends on wavelength, material thickness, cure profile, thermal exposure and the complete optical path. The datasets above should be used for application evaluation under their stated test conditions rather than as guaranteed transmission specifications for other assembly configurations.

 
Electrical Characterization

Dielectric constant and dissipation factor

Dielectric constant remains between 2.1 and 2.2 across the supplied 50 Hz to 1 MHz dataset. Dissipation factor decreases from 0.010 at 50 Hz to 0.005 at 1 MHz.

Frequency-dependent dielectric characterization
Frequency Dielectric constant Dissipation factor
50 Hz 2.1 0.010
1 kHz 2.2 0.006
100 kHz 2.2 0.006
500 kHz 2.2 0.006
1 MHz 2.2 0.005

Electrical-data limitation: The supplied dataset identifies frequency but does not provide specimen geometry, test temperature, cure condition, electrode configuration or measurement method. The values should not be extrapolated beyond the tested frequency range without additional validation.

 
Environmental Evidence

Bond-line observations after humidity and thermal storage

ABP 6892 demonstrated robust adhesion and a void-free bond line after the two environmental exposures below. The observations apply to the evaluated construction and test conditions and should not be interpreted as universal package qualification.

Humidity exposure

60 C / 90% RH

Exposure duration: 96 hours. Robust adhesion and a void-free bond line were observed after exposure.

High-temperature storage

120 C HTS

Exposure duration: 100 hours. Robust adhesion and a void-free bond line were observed after exposure.

Performance data and application validation

Optical, dielectric, mechanical and environmental results on this page represent performance under specific specimen dimensions, materials, cure conditions, aging exposures, frequencies, wavelengths and test configurations. Actual performance can vary with bond-line thickness, substrate, surface preparation, package geometry, optical path, cure process, temperature, humidity and assembly design. Customers should validate ABP 6892 under their actual manufacturing process and qualification conditions before production use.

 
Product Evaluation Support

Evaluate ABP 6892 for your sensor or optical assembly

Krayden can support evaluation of ABP 6892 for bond-line thickness, sensor-die geometry, jet dispensing, optical wavelength, cure profile and environmental requirements. Contact us to discuss technical data, samples, processing considerations and qualification planning for your specific glass, ceramic, wire-bond or optical assembly.

Contact Us

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers